Lead tinning has experienced a surge in popularity recently for a number of reasons, even though the process has been in use for nearly 25 years. The original need arose when the military decided that plated finishes, which are not fused, were not suitable or acceptable for high-reliability environments.

The problem, at the time, was that plated finishes were found not to be robust enough to withstand oxidation encroachment to the base lead, and could result in a solder joint failure in the field. That process gradually diminished in necessity over the years, but now it has come back along with several other circumstances that require hot solder dipping, better known as “tinning.”
So, there are essentially five basic reasons for re-tinning:
- Refurbishing of “legacy components” - Removing the oxidized (plated) lead finish and replacing with a fused intermetallic Sn/Pb finish;
- Gold embrittlement mitigation: Removing the gold from the components leads by “solubilizing” in molten Sn/Pb solder;
- Tin whisker mitigation: Replacing the tin plating with fused alloy;
- Converting RoHS components to Sn/Pb;
- Converting Sn/Pb components to RoHS.
1) First and foremost is the need to assure that older or legacy components that are designed into high-rel circuits are solderable. These components may have been inventoried for years under uncertain conditions, making the solderability of the terminations questionable. The molten solder dipping process will remove to old finish while applying a fresh “fused” SnPb finish.
2) The second occasion is to “scrub” the gold off component leads. Initially, gold is customarily plated onto component leads to help the base metal stand up to the rigors of various high-rel qualification processing. That gold must be removed and replaced with SnPb alloy because gold can cause “gold embitterment” in the solder joint if it remains.
3) The third reason for re-tinning is mitigation of tin whiskers, something everyone seems rightfully concerned about these days, in the conversion to high tin content lead-free alloys. Even NASA has published papers that say, in effect, that the only reliable way to mitigate tin whiskers and prevent their growth is to dip the leads in molten alloy. This creates a fused intermetallic finish that is unlike the non-fused electroplated finishes, which are a lot like a coating of sand--not fused or connected and prone to tin whisker development under certain conditions.
4) In the fourth instance, we remove or change the finish on a required component, when that component is not available, off the shelf, with the correct or specified finish allow. For example, let’s say I'm building a high-rel assembly that must be assembled using traditional lead-bearing Sn63 alloy. Unfortunately, the components that I need to use in that assembly are only available in a RoHS-compatible finish, in this case, electroplated tin. What do I do? The answer is to wash of the RoHS finish in the “scavenging” solder pot and apply the Pb finish in the second solder pot. Now those components are acceptable for my assembly (this can be verified with XRF or other means).
5) The fifth case is quite the reverse of the fourth, that is, to replace Pb finishes with a RoHS-compliant Pb-free finish. This operation, although similar to the fourth instance, requires special solder pots filled with RoHS alloy and constructed from titanium (this is the only proven non-contaminating material that is immune to the aggressive molten Sn).
These are the “whys” of re-tinning; however, the “hows” are critical to achieving success. There are several very fundamental requirements: Fixturing, flux application, pre-heating, removing the old finish and the final application of the fused solder alloy forming a non-porous intermetallic protective barrier.

Fixtures that accommodate all the various component body styles are necessary to hold and locate the components with the leads exposed to the flux and solder. The fixtures must be easy to populate yet precise, as the repeatable location is critical to depth of immersions. The exposed areas of the fixture should be made of titanium. Also consider that the fixtures may continue to hold the components through the post-cleaning step (if necessary) so plenty of drainage is good.
The choice of flux must match the activity needed to remove the old finish, and it must also match the best “wetting” to the base metal. This can vary considerably with aged components, so it is wise to use a wetting balance tester to determine these requirements as it is wise to test the fluxes before jumping into production. The wetting balance test will graphically demonstrate the best flux that is compatible with the component lead finish.
As an example, just arbitrarily using rosin flux on a legacy lead will likely not provide a satisfactory wetting curve, while an active flux will. With the flux chemistry in check, the application of the flux must be accurate and repeatable. Too much flux will cause unwanted residue on the component and contamination of the fixtures. If the fluxing is done just right, there should be little or no flux residue left and the solder finish should be bright and smooth.
Pre-heating is necessary to activate the flux. For most components, this can be achieved by hovering slightly above the solder pot. For heat-sensitive components it is best to hover over a forced hot-air station to ramp the body temperature to a safe level to prevent thermal shock. Both methods should be thermally profiled to ensure the correct temperature rate of rise.
There should be two separate solder pots used--one containing the ‘sacrificial’ alloy for scrubbing, and the second containing the “virgin” new alloy needed to coat the leads. The solder pots should be active or “flowing,” not a static solder pot. The flowing solder, particularly in the scrubbing pot, removes contaminated or scavenged material such as gold from close proximity to the leads, so that the contamination will not be pulled back to and deposited onto the component lead when the component is pulled out of the solder.
It’s also important to have some sort of agitation in the first (scrubbing) pot as this actually helps the removal of gold or lead solder from the leads. This can easily be accomplished with mechanical manipulation of the device holding the component in the bath. The use of nitrogen blanketing or inert atmosphere in the second (finishing) pot is desirable because it promotes a lustrous finish, and mitigates dross formation, as well as the formation of icicles and bridging.
To have a successful process, one must consider and control all of the above in an automated production environment with every process variable--dwell, temperature, depth, etc.--strictly regulated. This helps ensure that components will be processed in accordance with IPC/EIA JSTD-001 and ANSI-GEIA-STD-0006.
The procedure for re-tinning through-hole components, from start to finish, involves the following steps:
- Incoming solderability test using a wetting balance tester to determine the flux type;
- Careful handling and fixturing of the components;
- Processing the components in a robotic lead tinning system to control;
- Flux volume applied to the leads (chemistry pre-determined);
- Apply preheat (best to use forced heated air--not IR) to activate the flux and raise the component body temperature to reduce thermal shock;
- Solder dip--using a double dip process. The first dip is into a cleansing bath of molten alloy to remove the original coating, followed with a flux dip then a final immersion into a clean solder bath for a pure eutectic or RoHS finish;
- Post cleaning (if necessary);
- Visual inspection;
- Final wetting balance test to ensure best solderability;
- Lot report documenting the details of the process.
Conclusion
Removing gold plating, replacing RoHS finishes with Pb, refurbishing legacy components and tin whisker mitigation are the major reasons to hot solder dip component leads. Re-tinning of through-hole and SMT/QFP components is a robust and reliable automated process whereby component leads (or terminations) can be refurbished in preparation for re-qualification to high-rel standards, and helps ensure that components will be processed in accordance with IPC/EIA JSTD-001 and ANSI-GEIA-STD-0006.
Alan Cable is president of A.C.E. Production Technologies. He can be reached at 509-924-4898 or acable@ace-protech.com.