- News
- Books
Featured Books
- smt007 Magazine
Latest Issues
Current IssueSpotlight on India
We invite you on a virtual tour of India’s thriving ecosystem, guided by the Global Electronics Association’s India office staff, who share their insights into the region’s growth and opportunities.
Supply Chain Strategies
A successful brand is built on strong customer relationships—anchored by a well-orchestrated supply chain at its core. This month, we look at how managing your supply chain directly influences customer perception.
What's Your Sweet Spot?
Are you in a niche that’s growing or shrinking? Is it time to reassess and refocus? We spotlight companies thriving by redefining or reinforcing their niche. What are their insights?
- Articles
- Columns
- Links
- Media kit
||| MENU - smt007 Magazine
Low-Temperature SMT Solder Evaluation
July 5, 2019 | H. Osgood, D. Geiger, R. Pennings, C. Biederman, J. Jiang, and J. Bernal, Flex Inc.Estimated reading time: 5 minutes

Abstract
The electronics industry could benefit greatly from using a reliable, manufacturable, reduced-temperature, SMT solder material (alloy composition), which is cost competitive with traditional Sn3Ag0.5Cu (SAC305) solder. The many possible advantages and some disadvantages or challenges are discussed. Until recently, the use of Sn/Bi-based materials has been investigated with negative consequences for high strain rate (drop-shock) applications; thus, these alloys have been avoided. Recent advances in alloy “doping” have opened the door to revisit Sn/Bi alloys as a possible alternative to SAC-305 for many applications.
We tested the manufacturability and reliability of three low-temperature and one SAC-305 (used as a control) solder paste materials. Two of these materials are doped Sn/Bi/Ag, and one is just Sn/Bi/Ag1%. We will discuss the tests and related results. Lastly, we will discuss the prospects, applications, and possible implications (based on this evaluation) of these materials together with future actions.
Introduction
A typical SAC305 (Sn3Ag0.5Cu) reflow profile will have peak temperatures in the range of 235–245°C. Tin/bismuth or tin/bismuth/silver solder alloys may use a peak temperature in the range of 165–195°C. This represents a peak temperature delta of more than 50°C. Aside from the obvious energy cost savings, there are many other benefits to using a low-temperature solder (LTS) material, and they will be discussed later in this article. We also discuss some of the known and unknown risks as well.
Tin/bismuth and tin/bismuth/silver alloys are well-known to the industry and have been used routinely in consumer products that are not likely to be subjected to shock, drop, vibration, or high temperatures, such as TVs and some appliances. These alloys are more brittle than SAC-305 and more creep resistant. This makes them well-suited for low strain rate stresses (temperature changes) but not well-suited for high strain rate stresses (shock, drop, vibration, bend, etc.).
Some solder material suppliers have been working for several years to develop a version of this (low-temperature) alloy, which is comparable to SAC-305 in terms of higher strain rate reliability.
Historically, they had come close, but only recently have they hit the mark using “secret” recipes that include trace amounts of “dopant” materials to make the alloy more ductile and crack resistant. Other papers [1 & 2] discuss the dopant effects on lattice and grain structures by adding trace amounts of elements, such as copper, nickel, manganese, and antimony. We will not go into that detail here, but the main point is that some suppliers seem to have found an appropriate recipe that maintains the bulk alloy (and hence low melting point) but alters its properties in a sufficiently beneficial way.
Another key factor in our consideration was that there had to be more than just one supplier of these types of materials before we performed any serious evaluations. We tended to avoid embracing proprietary processes or materials, which are only available from a single source.
Advantages
Some of the possible advantages of LTS include:
• Reduced board and component warp
• Reduced head-in-pillow
• Lower residual stress
• Reduced pad cratering
• Reduced CTE geometrical effects (scale factor)
– Allows for smaller land pads/footprints
• Less expensive materials
– PCBs
– Components
• Less thermal exposure
– Thermally sensitive components
– Semiconductors
• Lower energy and maintenance costs
– Estimated 20–25% lower energy cost depending on the profile
– Lower maintenance cost on oven moving parts
• Possible hybrid assembly
– SAC-305 on one side and low temp on the other
• Reduced voiding
– ~50% void reductions observed
Disadvantages
As with any new material, there are unknown risks that may not come to light until the material is in use for some time. Some of the known risks include:
• Package warp—hot tearing
– Large BGA packages that were previously designed to flatten out at over 210°C can cause “hot tearing” in the solder joint because the package never completely flattens and remains warped throughout the reflow cycle. One remedy for this is to use more solder paste to make up for the gap difference. The lower-temperature alloys did not tend to wet as aggressively (discussed in more detail later) and therefore can allow more solder per unit area without bridging. If the industry moves towards accepting these alloys on a large scale, it is likely the packaging vendors will adjust accordingly and may offer “LTS” versions of these packages
• Rework
– Solder wire: Very limited (only one known source and it is not commercially available yet) and it is brittle
– Cracked solder pots: Bismuth expands when it cools, so it can cause some solder pots (wave solder) to crack
• Wide liquidus/solidus range
– We observed that a very rapid cooling was necessary to guarantee that the assembly was below 138°C exiting the conveyor reflow oven
• Flux residue
– We observed a considerable amount of flux residue after reflow. In time, these solder pastes may evolve to improve this
• More slump and less wetting
– Our tests indicate a bit more slump (hot and cold) than our controlled material, but again, this is more likely to do with the maturity of the paste. However, the alloy itself does not wet as aggressively as SAC-305, which can be an issue in certain circumstances, although we still found it to be acceptable. In some cases, less wetting can be an advantage as well, such as for paste in hole
Experimental and Results
Materials Tested
Figure 1 shows the materials tested.
Figure 1: Materials tested.
Material A is the control material. Materials B and D are the “doped” alloys, and Material C has no dopants added.
Assembly Conditions
All test boards were baked, inspected, and labeled before solder screen print. Solder paste inspection (SPI) was performed as well as SMT assembly and reflow.
Reflow Profile for LTS
Although peak temperatures as low as 165°C can be used (and should be used when appropriate), a higher temperature of 190°C was used to drive mixing on the SAC-305 BGAs. The solder paste and BGA ball interface experiences a sufficient phase change at these temperatures to drive diffusion and hence mixing of the BGA ball with the solder paste.
Mixing of the BGA with the SnBi paste was approximately 50%. This is comparable to Time 0 as well as a characteristic of all the solder joints we observed, which fell into the 40–60% mixing range.
To read the full article, which appeared in the July 2019 issue of SMT007, click here.
Testimonial
"We’re proud to call I-Connect007 a trusted partner. Their innovative approach and industry insight made our podcast collaboration a success by connecting us with the right audience and delivering real results."
Julia McCaffrey - NCAB GroupSuggested Items
Koh Young, Fuji, and Kurtz ERSA Drive Smart Manufacturing Solutions for EV and Automotive Electronics at Kunshan, China Technical Seminar
09/11/2025 | Koh YoungKoh Young Technology, the global leader in True 3D measurement-based inspection solutions, partnered with Fuji Corporation and Kurtz ERSA to host an exclusive technical seminar for leading automotive manufacturers in East China. Held on September 4 at Fuji’s factory in Kunshan, the event gathered participants representing over 35 companies.
MacDermid Alpha Presents at SMTA New Delhi, Bangalore Chapter, on Flux–OSP Interaction
09/09/2025 | MacDermid Alpha Electronics SolutionsMacDermid Alpha contributes technical insights on OSP solderability at the Bangalore Chapter, SMTA reinforcing commitment to knowledge-sharing and industry collaboration.
Electra’s ElectraJet EMJ110 Inkjet Soldermask Now in Black & Blue at Sunrise Electronics
09/08/2025 | Electra Polymers LtdFollowing the successful deployment of Electra’s Green EMJ110 Inkjet Soldermask on KLA’s Orbotech Neos™ platform at Sunrise Electronics in Elk Grove Village, Illinois, production has now moved beyond green.
Absolute EMS: The Science of the Perfect Solder Joint
09/05/2025 | Absolute EMS, Inc.Absolute EMS, Inc., a six-time award-winning provider of fast turnaround, turnkey contract electronic manufacturing services (EMS), is drawing attention to the critical role of 3D Solder Paste Inspection (SPI) in ensuring the reliability of both FLEX and rigid printed circuit board assemblies (PCBAs).
Indium Corporation to Highlight High-Reliability Solder Solutions at SMTA Guadalajara Expo
09/04/2025 | Indium CorporationIndium Corporation, a leading materials refiner, smelter, manufacturer, and supplier to the global electronics, semiconductor, thin-film, and thermal management markets, will feature a range of innovative, high-reliability solder products for printed circuit board assembly (PCBA) at the SMTA Guadalajara Expo and Tech Forum, to be held September 17-18 in Guadalajara, Mexico.